A battery tray and a battery case are not two names for one casting. Inside an EV battery housing, the tray carries the modules and ties the pack to the body while the case closes the volume and holds the leak rate. Put both jobs on one aluminium part and that is where most of the cost and most of the PPAP arguments come from.
What follows is the split we use when a Tier 2 customer sends one part number and expects one answer. The numbers are typical process windows from our 350T–3050T cells, not a claim about any single project. Where the two duties conflict, the article says which one wins rather than averaging them.
What is the difference between a battery tray and a battery case?
The tray takes the load path; the case takes the leak path. That split decides the alloy, the wall, the datum scheme and the inspection plan.
A tray is a floor with a perimeter frame. It locates the modules, carries the cooling plate and the busbars, mounts to the body, and in a cell-to-pack architecture becomes part of the body-in-white load path instead of a box bolted underneath. One industry glossary describes it the same way: a structural base with a floor and perimeter frame that takes the load path and the cooling integration. A battery case is a lid or a full enclosure: it closes the volume, carries the seal groove, takes the fastener clamp load, and gives vented gas somewhere to go. An EV battery housing can be either, which is why the drawing has to say which one it is.
Who carries the load, and why the tray is a beam
The tray carries it in bending, and section depth does more for stiffness than wall thickness ever will. A deep rib beats a thick wall at lower mass and with less metal to feed, which is why tray ribs are tall and sparse rather than short and dense.
The rib roots are the first place we look after a die trial. A rib tall enough to do the structural job sits at the end of the filling path, and the mass around its root is exactly where shrinkage porosity forms. High vacuum die casting removes gas porosity; it does nothing for shrinkage, which needs a thermal fix — an insert change, a local cooling circuit, or a thicker feed path. Confusing the two is the most common process mistake we see on tray programs.
What we commit to is the drawing: Cpk ≥ 1.33 on functional dimensions, 1.67 on safety-critical ones.
Who seals, and what a casting is allowed to promise
The case seals; the casting only gives the gasket a flat, stable surface to sit on. Flatness on the face that touches the gasket is the specification that matters, measured after ejection and after machining, never on the die.
On the seal face we hold 0.3–0.5 mm depending on part size. Past roughly 400 mm of face length the number needs a real conversation, because a large casting moves after ejection and again after the first thermal cycle in the vehicle. Casting the groove into the die and machining only the land is cheaper than machining the whole groove, but it moves the tolerance stack onto the insert, and a worn insert shows up as a gasket that leaks at one corner.

Two rules keep this honest. A casting does not have an IP rating; IP67 describes the closed pack as built, with its gasket, fasteners and connectors, and no die caster can certify it on a bare part. And the leak limit belongs to the customer: pressure decay between 0.3 and 1.0 bar is the band we usually see, with helium for tighter limits, but pressure, medium, hold time and reject value have to be on the drawing. Otherwise acceptance becomes a negotiation after the first shipment.
The methods are standardising. SAE J3277/1, published in January 2025, sets out recommended practice for liquid leak tightness of propulsion battery packs, and it is the document to align a pack-level specification with before it reaches a supplier. A caster can meet a pack-level method; it cannot invent one.
Who conducts heat, and what the casting actually contributes
The casting spreads heat; the cooling circuit decides how much of it leaves. A tray is a large aluminium plate with good in-plane conduction, which evens out hot spots and gives the cold plate a continuous path upward.
It is not a cooling system. Heat has to cross an interface — thermal paste, a gap pad, a bonded plate — and that interface is where the design is won or lost. A bond line that varies across the pack becomes a cell-to-cell temperature spread that no extra coolant flow fixes, and enclosure tolerances set that variation directly. So the gasket face and the cold-plate face deserve separate specifications.
Cast-in cooling channels are seductive because they remove a bonded interface. They also move the leak risk inside the part, where a pressure-decay test on the pack cavity will never see it. A cast channel needs its own test, a cleanliness check to VDA 19.1, and a wall that survives core shift.
One casting or a welded assembly
One casting wins on part count and datum consistency; a welded assembly wins on tooling cost and replaceability. Which is right depends on where the pack sits in the volume curve.
The monolithic argument is real: a single casting removes a weld line, a fixture and a stack of fasteners, and gives machining one datum instead of four. The bill arrives three ways — a die that may not fit the 3050T ceiling, a defect anywhere in a part that size scraps the whole thing, and a flatness that has to be held over an area no fixture can straighten.
The welded argument is equally real, and it is still the industry default. A 2025 study from the BCAST group at Brunel, in IOP Conference Series 1335, notes that EV battery boxes are built mainly from extrusions joined by welding, riveting or adhesive, with castings used sparingly because of lower performance and higher defect rates. Their answer was to cast the corner nodes, and X-ray tomography showed local porosity tracking local mechanical properties: the defect map and the property map are the same map.
That is what we usually recommend for large packs — cast the nodes and the floor, extrude the rails, and put the seal on a machined aluminium surface rather than a weld.
Tray and case side by side
The table separates the two jobs row by row, and the alloy row is where quotations most often go wrong.
| Item | Tray | Case / enclosure |
|---|---|---|
| Primary duty | Carries module mass, locates cells, ties the pack to the body | Closes the volume, holds the seal, routes vented gas |
| Dominant load | Bending and torsion from road input, jacking and crash | Fastener clamp load, internal pressure, lid stiffness |
| Alloy logic | ADC12 or A380 where stiffness per euro decides; AlSi10MnMg where the crash pulse needs 8–12% elongation | A380 or A360 where machining and sealing dominate; A356 only where a welded joint is required |
| Process window | VHPDC on 350–3050T, ribs and bosses in the die, single-setup machining of mounts | VHPDC, groove cast or machined, flatness recovered after ejection |
| Inspection | CMM on mounts and datum scheme, X-ray at rib roots per ASTM E505 | Profile and flatness on the seal face, 100% air-decay or helium on the closed assembly |
| Failure consequence | Module misalignment, cracked mount, noise path into the body | Water ingress, isolation resistance drop, blocked venting |
Read the alloy row twice. The tray is usually the part where elongation earns its cost, because the crash pulse reaches it first; the case is where machinability and dimensional stability earn theirs. Specifying AlSi10MnMg for the lid because the tray uses it buys elongation the lid does not need and costs flow length in a thin section.
How an airtightness test is actually set up
The test is a method, a fixture and a limit, and a drawing that names only the limit is not testable. Before a gauge is chosen, three things must be fixed: the volume being pressurised, the temperature at which it is measured, and whether the part is tested bare or assembled.
A bare casting test looks for a through-wall defect; an assembly test also covers the gasket, the weld and the connectors. A program that runs only the first discovers the second at the customer’s end-of-line.

The practical failure mode is rarely the leak itself. It is thermal drift: a part straight off a warm line, still stabilising inside the fixture, shows a pressure change that has nothing to do with a hole. Soak time and a reference volume fix more false rejects than a tighter gauge. Check the fixture with a calibrated leak once a shift.
| Method | What it registers | Typical setting | Blind spot |
|---|---|---|---|
| Pressure decay, air | Gauge pressure drop across a hold time | 0.3–1.0 bar test pressure, limit set by the customer | Temperature drift dominates when the limit is small against the volume |
| Helium, vacuum or sniff | Helium partial pressure through the leak path | Tighter limits than air decay, tracer at the joint | Cost per test, and tracer has to reach the defect |
| Proof / burst | Structural margin of the closed case | Customer-defined proof pressure | Proves a design once, not production conformity |
| Assembly water or dust test | The pack as built, to its IP rating | IP67 per the vehicle specification | Not a casting test, and one pass says little about ten years of service |
The last row is the one that gets argued about. An IP rating is a type test on a sealed assembly; a pass on day one does not describe the gasket after two hundred thermal cycles. Treat the production leak test as the control that keeps the process honest, and the type test as the qualification that opens the program.
Five design errors that show up in RFQs
Most avoidable cost on these parts is decided before the RFQ is sent.
- Flatness on the wrong face. A 0.3 mm callout on the raw casting and nothing on the machined land means the supplier optimises the wrong surface.
- Seal groove cast to final size in the draft direction. It inherits die wear and ejection history. Leave stock on the land and machine it.
- IP67 on the casting drawing. It cannot be certified there. Move it to the assembly drawing and keep a leak limit on the part.
- Ribs sized for stiffness with no feeding path. The rib root becomes the porosity site the crash model never saw.
- One leak limit for coolant channel and pack cavity. Different volumes, different acceptable rates; one limit forces the tighter onto both.
Frequently Asked Questions
Is a battery tray the same thing as a battery case?
No. The tray is the structural base that carries modules and mounts to the body. The case is the enclosure that closes the volume and holds the seal. In cell-to-pack designs the tray often becomes part of the body structure while the case may be no more than a lid.
Can a die-cast tray meet a pack-level leak specification?
The casting can meet a through-wall limit, and we test 100% of them for it. A pack-level limit also covers the gasket, the weld and the connectors, so it belongs on the assembly drawing. Give the casting a pressure-decay limit in the 0.3–1.0 bar band with a defined hold time.
Why not cast the whole enclosure in one piece?
Above a certain pack size the die and the machine become the constraint, and one defect scraps a part that already carries an hour of machining. A hybrid — cast floor and nodes, extruded rails, machined seal land — usually costs less per good pack, even with an extra supplier.
Which alloy should a tray use?
Start from the failure mode. If the tray only has to stay stiff and locate modules, ADC12 at 230–310 MPa or A380 at 315–325 MPa does the job at the lowest cost per kilo. If it has to bend before it breaks, AlSi10MnMg at 8–12% elongation buys that behaviour and costs more.
How flat does the seal face need to be?
0.3–0.5 mm across the face, depending on length, measured after machining. Beyond about 400 mm the number has to be agreed against the die design, because a large casting keeps moving after ejection and again after the first thermal cycle.
What the casting does, in the end, is decide which job gets the tight tolerance. Put the seal on a machined land, put the stiffness in the section depth, and keep the pack-level test on the assembly drawing where it can be run. A drawing that separates those three is cheaper to quote and much harder to argue about at PPAP.
The material side of the same decision — where steel still wins on cost per kilo and aluminium wins on mass — is in aluminium versus steel for EV battery housings.