Integrated die casting fails in four places, and the press is not one of them: the die, the vacuum system, the heat treatment furnace and the scrap account. A 9,000 t machine closes on command; what it closes on is one casting carrying the cost of every part it replaced, so porosity that would scrap a 2 kg housing scraps a 60 kg rear structure with machining capacity already scheduled behind it.
The ramp numbers explain the caution. A 2025 Euroguss expert interview on megacasting puts scrap at up to fifty percent during ramp-up and the capital for a couple of complete lines at €60–80 million. That combination is why the technology moved through greenfield plants before existing body shops.
This is for Tier 2 and Tier 3 suppliers asked to quote around these programmes, and for buyers deciding whether the architecture fits. Our ceiling is 3,050 t, so we make the housings, brackets and machined inserts around a giga structure rather than the structure itself; automotive die casting at that scale is what we quote from.
Where the process actually breaks
It breaks at the last-filled end of the cavity, at every thick-to-thin transition, and in the furnace after the part has already passed X-ray. A single-piece structure removes the buffer a welded assembly provided: when one bracket was out of tolerance, the bracket was scrapped; when one feature of a 2 m casting is out, the whole casting goes, or someone starts asking whether it can be welded.
The defect map is not random. Metal that arrives last is colder and has pushed air ahead of it; sections that change thickness cool at different rates; and any gas left in the wall expands when the part is reheated.
| Failure mode | Where it is found | Physical cause | Mitigation that works |
|---|---|---|---|
| Gas porosity at the last-filled end | X-ray, machined section, leak test | Air and gas pushed ahead of cold metal | Cavity vacuum logged per shot, vents at the last point to fill |
| Shrinkage porosity in thick sections | CT, or a machined face after exposure | Isolated feeding across a thick-to-thin step | Local squeeze, die thermal balance, wall redesign |
| Elongation gradient along the part | Tensile coupons cut from both ends | Transition point and fill pattern differ end to end | Transition position on the control plan, load path where ductility is proven |
| Blisters after solution treatment | Furnace exit, visual inspection | Entrapped gas expanding at solution temperature | T5 or shortened T6, lower gas content, dry shot |
| Distortion after quench | CMM after machining | Residual stress releasing in the cut | Fixture quench, stress relief, allowance on functional faces |
| Repair rejected at audit | PPAP review, customer source inspection | Welding prohibited on crash-relevant castings | Written scrap policy, design for bolted replacement |
None of that is fixed by a bigger press, and each mechanism has its own instrument, from a cavity trace to a CT scan.
Machine and tooling scale: what a 9,000 t line changes
A 9,000 t line is a different building rather than a bigger cell: 6,000–9,000 t of clamping force in current production, templates up to 6,500 × 5,800 mm, and a die whose mass sets the crane, the floor and the maintenance plan.
| Item | 3,050 t cell | 6,000–9,000 t integrated line | What it does to the programme |
|---|---|---|---|
| Clamping force | 3,050 t ceiling | 6,000–9,000 t in production; 16,000 t class installed | Die structure is sized for the load, not adapted to it |
| Template and footprint | Standard platens | Up to 6,500 × 5,800 mm | Building height, foundation and crane enter the quote |
| Platen deflection | Small against a 1.5–2.5 mm wall | 0.8–1.2 mm at cavity centre at 9,000 t and 140 MPa | Wall thickness varies across the part unless the die compensates |
| Tooling | One die per housing, often two cavities | One die per structure, single cavity, no sharing between variants | Die build and tryout lead time delays SOP; cost amortised over one programme |
| Line capital | Cell-level investment | €60–80 million for a couple of lines | Volume threshold before piece price falls |
| Ramp scrap | Part-dependent and manageable | Up to 50% during ramp-up | Metal, energy and a machining slot in every scrapped part |
| Repair route | Weld, impregnate, re-machine | Replacement, rarely repair | Service and insurance cost moves back to the OEM |

The platen is part of the tolerance stack. On a 9,000 t machine, template deflection at the cavity centre reaches 0.8–1.2 mm at 140 MPa specific injection pressure, according to a 2026 review of integrated die-casting body structures. That is the same order as the wall tolerance on the drawing, so the die has to compensate for the machine rather than the operator compensating for the die.
A structure die is single-purpose, cannot be shared with the next model, and its build starts months before SOP. Every correction after tryout changes the casting, sending the part back through dimensional layout, X-ray and often a fresh PPAP submission.
Porosity and elongation: the limits that choose the alloy
Below 0.5% volumetric porosity and above 10% elongation are the two numbers a crash-relevant casting has to hold, and both are set by the shot rather than by the alloy certificate.
AlSi10MnMg with a controlled Fe/Mn ratio can reach 300 MPa and more than 10% elongation, which is why it became the default for these parts. The same review notes that 2–3% porosity cuts tensile strength by 10–30%, so a casting that looks acceptable on a sectioned sample can be a fifth short on the property the crash model assumed.

The far end of the part is where that shows up. In a 2024 study of a large one-piece Al-Si-Mn-Mg casting, moving the high-speed transition point from 1200 mm to 1160 mm raised elongation at the near end from 6.57% to 8.82% — a 40 mm change in the shot profile worth 25% more ductility — while the far end stayed at 3.8–4.1%. Same die, same alloy, same machine. The two ends of one casting do not have the same material, and the drawing should say which end carries the load.
Cavity pressure is the lever that works on gas porosity. The same study ran the cavity below 50 mbar with the shot chamber below 300 mbar, and vacuum at that level is a per-shot measurement rather than a pump specification. Shrinkage porosity is a different defect with a different fix, and identifying and controlling porosity starts with telling the two apart before anyone touches a setpoint.
Heat treatment is where the business case usually dies
T6 buys strength and ductility and, on a large thin-walled casting, it also buys blisters and distortion, which is why some giga structures are specified T5 or a shortened T6 instead of a full solution treatment.
A blister is gas already in the wall, expanded at solution temperature and pushed against a skin that has gone soft. No furnace atmosphere removes it, and no straightening recovers a face that bubbled under a sealing surface. The review is direct: distortion and blistering come from entrapped gas, and the alternatives are T5 aging or an optimised anneal.
Distortion is the slower cost. A 2 m part quenched from solution temperature carries residual stress that releases during machining, so holes move after the fixture is unclamped. Fixture quenching, a stress-relief pass before finish machining and typically 2–4 mm of allowance on functional faces are the usual defences, and each is cheaper than scrapping a finished part.
Repair, scrap and the cost of one bad shot
A scrapped structural casting carries the metal, the melting energy, the die time and the machining slot, and it usually cannot be welded back into a crash path, which is why a 50% ramp scrap rate is an architecture problem rather than a housekeeping problem.
Impregnation seals a leak path but does not restore elongation, and a part that needed it already had porosity above the limit. Welding is used in some non-structural repairs, but the Euroguss interview makes the downstream point: repair shops and insurers struggle with these parts because damage is hard to repair and expensive to replace.
Scrap rate is a process signature before it is a cost line: it responds to die thermal balance before operator discipline, and die thermal balance and scrap rates sets out where the losses originate.
Why single-piece rear structures fit some OEMs and not others
They fit an OEM with one high-volume platform, few body variants, a plant built for the floor load and a repair strategy that accepts replacement; they do not fit a low-volume, multi-variant line.
- Volume on one geometry. The die is single-purpose, so piece price only falls once it is spread over hundreds of thousands of parts.
- Variant count. A long-wheelbase version, a pickup bed or a second battery size usually means a second die.
- Crash and repair policy. If insurers in the main market will not accept replacement economics, the architecture creates a cost the OEM did not have.
- Plant and logistics. A 2 m casting needs crane capacity, floor space and a machining line close enough that transport does not eat the tolerance.
- Integration target. Casting into the battery case only pays when the surrounding structure is designed for it; bolting a giga casting into a legacy body gives the weight back.
The hybrid answer is often the right one: in the same review, the MeGiCast consortium found that a large casting with optimised sheet-metal reinforcement beat either pure casting or pure stamping on weight-performance, a quieter conclusion than press builders tend to give.
Where a programme sits on those five points decides whether a Tier 2 is quoting a structural part or a science project. Where HPDC stops for aluminium structural components is the boundary we use when a drawing arrives with a 1.8 m footprint.
How a Tier-2 supplier should qualify for a giga programme
Qualify the evidence, not the tonnage: a supplier with a 9,000 t press, no per-shot vacuum record and no CT is less capable than one with 6,000 t and a validated window.
- Vacuum at the cavity, logged per shot. Ask for the trace rather than the pump rating; below 50 mbar at the cavity is the number the structural studies work to.
- Transition position as a controlled parameter. A 40 mm shift changed elongation by a quarter in the study above, so the setting belongs on the control plan, not a setup sheet.
- X-ray or CT sized for the part. A 2 m casting does not fit every cabinet; agree the sampling, the standard (ASTM E505 for aluminium castings) and the acceptance images before the first shot.
- Heat treatment under control. Furnace class, fixture, quench delay and distortion record per batch; if the drawing says T5, the supplier should explain why, not just comply.
- A dimensional strategy for 2 m. Datum scheme from cast features, CMM capacity, and Cpk at or above 1.33 on the functional dimensions rather than the easy ones.
- A written scrap and repair policy. What is impregnated, what is welded and where, what is scrapped; without it every nonconformance becomes a negotiation.
- PPAP Level 3 on a part this size. Control plan, PFMEA and MSA built around the real process, not a template copied from a 2 kg housing.
Most Tier 2s will not have the press, and that is not disqualifying. Machining, leak testing, sub-assembly and the smaller structural parts still run on a 350–3,050 t cell, judged by the same evidence. Our quality control is built on that chain: per-shot process data, CMM layouts and a PPAP file a customer can audit rather than admire.
If a drawing arrives at 9,000 t, the honest answer is that we are not the press for it. The useful answer is which parts of that programme we can hold, and what the Tier 1 should ask the giga caster before it signs the tool.
Frequently Asked Questions
What clamping force does integrated die casting need?
6,000–9,000 t covers the rear and front structures in production today, with machine classes to 16,000 t installed for larger parts; below 6,000 t, projected area and shot weight limit what can be made in one piece.
Is an integrated casting cheaper per part than a welded assembly?
Only above a volume threshold. The die and the line are fixed costs and ramp scrap is carried by early production, so a low-volume programme pays more per part than the assembly it replaced.
Can a large structural casting be T6 heat treated?
It can, but the risk is blisters and distortion rather than insufficient strength. Entrapped gas expands at solution temperature, so many programmes specify T5 or a shortened T6 and accept lower elongation for a flat part.
Can a crash-damaged integrated casting be repaired?
Rarely. Replacement is the normal route, which is one reason insurers and repair shops treat these structures cautiously. Leaving bolted, replaceable sections around the casting reduces the exposure at some cost in parts count.
The press is the easy part of the investment. What decides whether a giga programme ships is whether the vacuum trace, the transition window, the heat-treat record and the scrap policy were proven on the same part, and whether volume paid for proving them.