An engine bracket is the easiest part in an RFQ package and the hardest to get signed off. It has no sealing face, no bearing bore and nothing cosmetic, so it gets the least engineering attention in the project — and then it cracks at 180,000 km because nobody wrote down which loads it was supposed to survive.
I quote brackets for European Tier-1 programmes, and the quote changes by 30 % depending on how three questions are answered: what load path the bracket sits in, what elongation the alloy has to deliver, and how much of the mounting geometry is machined after casting. This is how I work through those three before the die is cut.
What a bracket actually carries
Four load families arrive at the same casting, and each pushes the design in a different direction. Treating them as one “strength” requirement is the most common mistake I see in drawings.
| Load family | What it does to the part | Design answer |
|---|---|---|
| Assembly preload | Compressive stress under the bolt head, creep if the boss is thin | Boss height at least 1.5× bolt diameter, spot-faced top, no drafted seating ring |
| Torque reaction | Fully reversing load, 106–107 cycles over life | Ribs aligned with the load, generous internal radii, no sharp intersections |
| Vibration | Amplified displacement if the first natural frequency sits below engine order excitation | Diagonal rib to raise stiffness, mass kept near the mounting plane |
| Thermal cycling | Differential expansion against steel bolts and a hotter block | Slotted or oversized clearance holes, avoid a two-bolt pattern that fully constrains expansion |
The pattern that fails is always the same: a bracket that is stiff in the static case, has a natural frequency just above idle, and then sees its worst stress at 2,300 rpm in third gear. A static FEA pass will not show it.
Why cast instead of fabricated
Twenty years ago this part was a steel fabrication: two pressings, a welded tube and a machined pad, six to twelve welds, and a fixture for each operation. A single aluminium die casting replaces that assembly with one part that is 40–50 % lighter and does not need a weld inspection plan.
What makes the business case work is not the weight. It is the removal of operations. One casting means one incoming inspection, one fixture family, one dimensional report, and no weld distortion to chase during the PPAP run. On a bracket with a total spend of a few euros per part, that overhead is often larger than the material saving.
Fabrication still wins in two cases: below roughly 3,000 parts a year, where the die cannot be amortised, and where the bracket has to be welded to a steel subframe, which brings the joining problem back anyway. For the structural castings that sit next to these brackets in an EV programme, the same volume logic decides the process — I go through it in aluminium structural components for EVs.
The alloy decides the elongation budget
Fatigue in a casting does not start in the bulk metal. It starts at a stress raiser: a gas pore, a shrinkage cavity, a cold shut, or a corner that was drawn as an internal right angle. The alloy decides how much of that damage the part can absorb before the crack runs.
ADC12 and A380 are the default because they cast thin walls and fill complex geometry easily. Their elongation is 1–3 %, which is fine for a bracket that is loaded in compression and barely fine for one that reverses load. A primary alloy such as AlSi10MnMg, in a T7 condition, buys 8–12 % elongation and a higher fatigue limit, at the cost of tighter process control: those alloys are less tolerant of gate design and die temperature, and the heat treatment adds a distortion step that has to be straightened.
| Alloy | UTS | Yield | Elongation | Where it belongs |
|---|---|---|---|---|
| ADC12 | 230–310 MPa | 150–170 MPa | 1–3 % | Covers, housings, brackets loaded mainly in compression |
| A380 | 300–320 MPa | 160 MPa | 1–3 % | General purpose, good machinability, generous sections |
| AlSi10MnMg, T7 | 260–300 MPa | 200–240 MPa | 8–12 % | Structural brackets with a real fatigue duty |
| A356-T6, squeeze cast | 280–300 MPa | 220–240 MPa | 6–10 % | Low volume, highest integrity, thick sections |
Those are typical ranges from alloy datasheets, not measurements from one lot. The point of the table is the trade, not the third digit: every step down that list buys ductility and pays for it in castability, cycle time or tooling cost.
Vacuum assistance is worth mentioning here because it changes the fatigue result without changing the alloy. Work published on vacuum-assisted HPDC with AlSi10MnMg shows the defect population — and with it the fatigue behaviour — responding strongly to both the vacuum level and the subsequent heat treatment (Metals 13(2), 389). If a bracket has a fatigue requirement, the vacuum level belongs in the purchase specification, not in the supplier’s process sheet alone.
Ribs and bosses: stiffness comes from geometry
A bracket’s stiffness at its root is set by the second moment of area, which is a geometry argument, not a thickness argument. Adding 1 mm to the whole wall costs weight everywhere and buys little; adding one 8 mm rib along the load line buys most of the stiffness for a fraction of the mass.
Four rules cover most of the design work:
- Rib thickness 0.6–0.8× the adjacent wall. A rib as thick as the wall creates a hot spot and pulls shrinkage porosity into the junction.
- Rib height no more than 5× rib thickness, with 1–2° draft and at least 0.5 mm radius at the base. A sharp base is a crack starter.
- Boss outside diameter 2–2.5× the hole diameter, with a height limit of about 3× OD before it needs a supporting rib.
- Internal radii 1 mm minimum everywhere, 2–3 mm wherever the load reverses. That is a tooling-cost decision as much as a strength one, because every radius has to be cut into the die.
The other lever is where the mass sits. A bracket with its mass concentrated near the bolted face and a thin, tall web out to the load point will ring at a lower frequency than the drawing suggests, because the web behaves as a plate, not a beam.
Holes, threads and inserts
Three options exist for every threaded connection, and the choice is driven by cycle count as much as by strength.
A cored hole that is later machined and tapped is the normal route: the die leaves 0.3–0.5 mm of stock, the machine shop drills, taps and controls position. It costs a machining operation but gives a thread you can inspect and repair.
A cast thread is cheaper and almost always a mistake. The die cannot hold the minor diameter through its life, the thread form is draft-limited, and the first repair oversize usually cracks the boss.
Cast-in inserts — steel or brass, moulded into the casting — solve the wear problem and create a thermal one: the insert shrinks away from the aluminium as the part cools, so the boss has to be designed as a shrink-fit ring, not as a hole. If the insert can rotate or pull out under torque, the design is wrong, not the insert.
For brackets that see repeated assembly at the OEM, a thread insert (Helicoil type) installed after casting is usually the cheapest reliable answer: the casting stays simple and the thread is repairable.
Tolerances that actually matter
Nobody inspects the general tolerance block on a bracket. Three dimensions decide whether it fits, and they should be called out individually rather than left to the title block.
Mounting face flatness. 0.2–0.3 mm over a 100 mm face is achievable as-cast on a well-cooled die; anything tighter goes to machining. A bracket that is bolted down over a warped face preloads itself and loses fatigue life before it ever sees a service load.
Hole position. ±0.15 mm after machining is a normal call for bracket holes; ±0.3 mm as-cast is realistic for a cored hole. Mixing the two in one pattern is how assembly fixtures end up fighting the part.
Hole-to-hole distance. This is the dimension that actually controls assembly, and it is the one most often left as a general tolerance. Put it on the drawing with its own value. The general treatment of as-cast versus machined tolerance bands is in tight tolerances in aluminium die casting.
Porosity and fatigue
A bracket fails by fatigue, and fatigue starts at a pore. That makes porosity a structural acceptance criterion on this part family, not a cosmetic one — which is a different conversation from the one most suppliers are used to having about housings.
Two defect types matter. Gas porosity comes from air trapped in the shot and sits where the flow front closed. Shrinkage porosity comes from a section that solidified last without a feed path, typically a thick boss or a rib junction. Both are visible on a radiograph, and both reduce fatigue life far more than their area fraction suggests.
What I put in the specification: radiography or CT on the first article and a sample per shift thereafter, with acceptance levels agreed against a reference standard rather than described in words. “No porosity in critical areas” is not an acceptance criterion, because the inspector cannot measure it. The sampling logic that works for castings in series is set out in incoming inspection of aluminium die castings.
Tooling and the volume threshold
A single-cavity die for a 500–900 g bracket typically runs 18,000–35,000 EUR depending on slider count, and a second cavity adds roughly 60 % of that again. The die life is 80,000–150,000 shots on a well-maintained tool, which puts the tooling cost at 0.20–0.40 EUR per part over a 100,000-part programme and at 2–4 EUR over a 10,000-part one.
That arithmetic sets the break-even against fabrication. Somewhere around 5,000–8,000 parts a year, the die stops being the dominant line in the quote and the casting becomes the cheaper route. Below that, a machined billet bracket or a small fabrication is usually the honest answer, and a supplier who quotes a die anyway is buying the order with your money.
What to put in the RFQ
Six lines turn a bracket RFQ from a price into a design review:
- The load case, in one sentence: what pulls on the bracket, in which direction, and how many cycles.
- The alloy and temper, or the elongation you need — not “aluminium”.
- Which faces and holes are machined, and which are as-cast.
- The three critical dimensions with their own tolerances.
- The porosity acceptance standard and the inspection frequency.
- Annual volume and expected programme life, because they decide the cavity count.
Where the bracket is part of a larger structural assembly, the process choice moves too — squeeze casting enters the picture when the section is thick and the fatigue duty is high, and I compare the two in squeeze casting versus HPDC.

Frequently Asked Questions
Can a die-cast bracket replace a welded steel bracket directly?
Only after the stiffness is re-checked. A casting is usually thicker in the web and thinner at the corners than the steel part it replaces, so the static strength matches while the first natural frequency drops. That frequency, not the yield strength, is what decides whether the swap works.
What elongation should I specify for a bracket?
If the load reverses more than 105 cycles, specify 8 % minimum and expect to pay for a primary alloy and a heat treatment. If the bracket is loaded mainly in compression by bolt preload, ADC12 at 1–3 % is adequate and much cheaper.
Do brackets need heat treatment?
Only if the alloy needs it to reach the specified elongation, which means the AlSi10MnMg family. ADC12 brackets are used as-cast. Heat treatment buys ductility but adds distortion, so a T7 bracket usually needs a straightening fixture and one more dimensional check.
How many cavities should the die have?
One, until the annual volume passes roughly 50,000 parts. A second cavity raises output and lowers the per-part machine cost, but it also doubles the die investment and makes the process window harder to hold on a thin-walled part.