Aluminum Die Casting Drawing Requirements: What to Specify

A drawing arrived last month with one line in the title block: no porosity in critical areas. No datum scheme, no zone map, no level. Three suppliers quoted three prices, each reading “critical” differently. The automotive part was not difficult. The drawing was.

Datums first: a casting has no natural zero

Fix the datum scheme before any dimension, because without it every inspection result is an opinion.

Cast surfaces move. A datum on a drafted wall or a raw parting line shifts between cavities and tool revisions, so fixture and CMM disagree from the first sample. Use a machined face or a datum pad as primary, a secondary that locks rotation and a tertiary that fixes the last degree of freedom. Confirm all three are reachable in the die, the trim fixture and the machining fixture; if not, the datum belongs on a cast pad machined later.

NADCA’s 2024 Product Specification Standards added a section on datum location next to its GD&T chapters.

ADC12 die casting drawing with datum callouts beside a machined aluminium housing and calipers

Draft angle: outer walls and cores are not the same problem

Draft is a separate value for every wall.

In a high pressure die casting, an outer wall slides off the cavity at a typical 1–2°. An internal feature is pulled by a core and the metal shrinks onto it, so the same depth needs 1.5–3°. Both depend on depth, surface and whether the face is machined; a 60 mm pocket at 1° is not a 6 mm step at 1°.

One degree over 120 mm of wall gives about 2.1 mm of clearance per side. Halve it and the part rubs the die over its full height, which shows up as drag marks and, at a corner, a tear in the usual defect list for automotive castings.

FeatureTypical valueWhat it depends on
Outer wall, as-cast1–2°Height, texture, ejection
Inner wall pulled by a core1.5–3°Depth, shrink onto the core
Deep pocket, over 50 mm2–3° or moreDepth, polish direction
Machined face0.5–1.0 mm stockTolerance grade, flatness, cleanup
Internal corner radiusAbout half the wallSection, stress, metal flow
Aluminium die casting clamped on a CMM fixture with the probe touching a machined bore

Machining stock and wall thickness belong on the same sheet

Allowance is drawn per face, not as a global note. 0.5–1.0 mm per machined face is typical, enough to clean up cast skin and flatness without turning a 2.5 mm wall into a 1.5 mm one. The allowance matches the as-cast grade, written per ISO 8062-3; a blanket ±0.05 mm is a machining tolerance, not a casting one.

A 2.8 kg ADC12 housing sits in the 1.5–2.5 mm band, with 1.2 mm possible on short local runs; under 1.2 mm is a separate evaluation. An internal corner with no radius is a hot spot and a stress riser, so draw at least half the local wall, 0.75–1.25 mm here, with a radius at every rib root.

Ejector pins and the gate have to be located, not tolerated

Mark where a pin mark or gate vestige is allowed and give a height; “minimal” cannot be inspected.

Every part leaves the die on pins and carries a gate scar. Zone them: no pin on a sealing land, datum face, bearing bore or visible Class A surface; pins on non-functional ribs and bosses. Then a number: flush to 0.2 mm proud on a non-sealing cast face is a common callout, flush on any face machined afterwards. Gate position is tooling; the residual height and the face it sits on are drawing decisions.

Porosity acceptance is a test, not an adjective

“No porosity” cannot be measured. A drawing that works names the method, the zone and the level.

Radiography gives a 2D projection of voids; CT gives a 3D map and wall sections. Either needs a target. ASTM E505 supplies reference radiographs with severity levels for aluminium die castings, so a usable callout names the level per zone instead of a bare “per E505”: A for a sealing land or bearing bore, B for a structural rib, C for a non-functional boss. CT also catches a pore that only reaches the surface after the boring bar, so machined parts are sampled after the cut.

Tightness is a separate callout. A part can pass radiography and still leak at 0.5 bar, so the drawing also names the pressure test method and leak limit.

Drawing itemWhat we see when it is missing
Datum schemeFixture and CMM disagree; first article argued
Draft per surfaceDrag marks, tearing, tool rework after T1
Machining stockThin wall after cleanup, cast skin on a seal face
Pin and gate zonesPins in a seal groove, rework or scrap
Porosity zone and levelTwo verdicts, a batch rejected at the customer
Alloy and temperWrong chemistry supplied “to the number”
Coating mapCoating under a ground strap, bare edge after masking

GD&T: tolerance the machined features, not the whole part

Position for bores and bolt patterns, profile for sealing faces, flatness where a gasket lands: 0.3–0.5 mm depending on face size. State ASME Y14.5 or ISO 1101, because the datum conventions are not interchangeable. Capability is Cpk ≥ 1.33, 1.67 on safety parts, attached to a short list of features. Tightening every dimension adds inspection and scrap.

Alloy, temper and finish: name the standard and map the surface

ADC12 and A380 are not interchangeable labels, and neither means anything without its standard.

The same chemistry is ADC12 in JIS H 5302, A380 in ASTM B85, and an EN AC grade in EN 1706. “ADC12 or equivalent” invites substitution the buyer did not intend. Write the designation, the standard, the year and the temper, because as-cast or T5 changes dimensions and cost. Then the values: ADC12 runs 230–310 MPa, A380 315–325 MPa, and AlSi10MnMg 250–280 MPa with 8–12% when the part must bend before it breaks.

Shot blast, passivation, powder coat, e-coat and laser marking are in scope; anodising a high-silicon casting is decorative at best. Mark which faces are coated, masked or machined after coating: a ground pad under powder coat is a resistor.

When the drawing and the process disagree

Most conflicts are geometry: a 0.8 mm wall beside a 4 mm boss, a pin on a sealing land, a tolerance that needs a second setup. We return numbered comments with a sketch, the reason and three options: change the part, change the process, or accept more scrap. The customer signs one; that version goes into the PPAP file, the tool drawing and the inspection plan.

We do not move a gate or add a pin and tell the customer afterwards. Scrap from a mismatch is charged to somebody, and it shows up in the rejection and rework rates before anyone admits the drawing was wrong.

What to send with the drawing

A PDF alone slows the quote down. The package we can cost in a day is short: a 3D model in STEP or IGES, the 2D drawing with datums and GD&T, the material and temper callout by standard, the finish specification, and the acceptance level for porosity or leak. Add annual volume and the expected model life, because both decide cavity count and whether a second die is worth planning.

Two things are often missing and change the price. First, which surfaces are cosmetic and which are only functional; a drafted wall that will be painted can carry a lower cosmetic grade than one that stays bare. Second, who owns the tooling and where it will be maintained. If the die moves to another plant later, the drawing has to travel with the same datum scheme, or the first parts off the second press will not match the PPAP submission.

Send the drawing before the RFQ, not after. A datum note changed at quotation stage costs nothing; the same note changed after the die is cut costs a tool revision and a fresh layout.

FAQ

What is the minimum information a die casting drawing must carry?

Datum scheme, alloy with standard and temper, draft per surface, machining stock and cut faces, wall and radii, pin and gate zones, porosity method and levels, the coating map, and the GD&T standard.

Can draft angle be left to the toolmaker?

No. Draft depends on depth, surface and whether a core pulls it, and it changes wall section and ejection force. Set by habit, it costs tool time after T1.

Is ASTM E505 enough as a porosity specification?

Not on its own. E505 gives reference radiographs and severity levels; the drawing must name the level per zone, the method, the sampling rate and where the sample is taken.

Who owns the problem when a casting cannot meet the drawing?

The customer owns the requirement, the foundry owns the DFM note. That split only works if the comment goes out in writing before steel is cut and the decision is a drawing revision.

A drawing that can be quoted without a phone call is the goal: datums that exist in the die, draft with a number, stock per face, pin and porosity zones, an alloy written with its standard. Everything vague becomes a first-article negotiation.