Pressure Testing of Aluminum Die Castings: Methods & Limits

A housing passed air decay at 0.5 bar, 30 seconds, 5 cc/min. The customer’s end-of-line rig at 1.2 bar found a leak in the first ten parts. Both were called a pressure test.

A pressure test proves only what its own settings say: a medium, a pressure, a dwell and a leak limit. Change one of the four and you are describing a different part. This page covers the four methods we run, how pressure and limit are set, where die castings actually leak, and what belongs on the drawing so the test means the same thing in our plant and in yours.

What a pressure test proves, and what it does not

It proves the part holds a defined pressure with a leak below a defined limit for a defined time. It does not prove the wall is free of porosity, and it does not predict behaviour above the pressure you tested.

A casting with a pore chain that stops 0.3 mm short of the far surface passes every air test and still fails after machining, because the boring bar opens the last 0.3 mm. A structural pore that never forms a through-path also passes, then fails a fatigue or burst requirement it was never tested against. So pressure tightness and internal soundness are two callouts, measured two ways. The porosity side is written on the die casting drawing; this page is the tightness side.

Four methods, four different answers

Pick the method from the smallest leak you must reject, not from the rig you already own.

MethodTypical rangeCycleWhat it is good forBlind spot
Air decay (pressure decay)0.3–1.0 bar; limit 0.5–5 cc/min15–60 s100% end-of-line on housings and coversLarge internal volume hides small leaks; temperature drift moves the reading
Pressure hold with flow meter0.3–2 bar; 0.5–10 cc/min20–60 sProcess control, trend charts per shiftNeeds a stable supply; leaks in the rig look like leaks in the part
Bubble immersion0.2–0.5 bar1–5 minFinding where the leak isOperator-dependent; too slow for 100% sorting
Helium mass spectrometry1×10⁻³ to 1×10⁻⁶ mbar·L/s1–10 minSealed cavities, validation, tight specsCost, background helium, part must be dry and clean

Units are where specs go wrong. 1 mbar·L/s equals about 59 cc/min, so a 1 cc/min limit is roughly sixty times tighter than a 1 mbar·L/s limit. A purchase order that mixes the two, or drops the unit, is not a spec. Convert to one unit before you compare two suppliers, and write the unit next to the number.

Aluminium die casting held in a bubble test tank with air bubbles rising from a corner seam

Pressure, dwell and the volume trap

Set the pressure from the service condition, then check the fixture can hold it without deforming the part.

For a sealed electronics or battery housing, 0.3–1.0 bar of dry air is the usual band: enough to open a pore path, low enough that a 1.5 mm wall and a lip seal are not pushed around. For a fluid channel, the callout is usually 1.5× the maximum working pressure, run hydrostatically, because air stores energy and a failure at 4 bar is not a test you want next to an operator.

The dwell has three parts and they are not interchangeable: fill, stabilise, measure. Skip the stabilise step and the reading is still catching up with the adiabatic heat of compression. A 1 K shift in part temperature moves the reading by about 3.4 mbar at 1 bar, which is more than most leak limits, so parts come off a warm die or a washing line and sit on the fixture until they are within a degree of ambient.

Volume decides sensitivity. The same 2 cc/min leak drops the pressure faster in a 200 cc sensor body than in a 3 L empty pack, because the pressure change is divided by the trapped volume. Either set the limit per part family after a known-leak test, or run a master leak on the rig at the start of each shift and chart it. Without that, a passing trend can be the rig drifting, not the process improving.

Where an aluminum die casting leaks

Most failures come back to five paths, and only two of them are casting defects in the narrow sense.

PathHow it shows in the testWhat to change
Interconnected porosity through the wallSteady leak, repeatable at the same spotVacuum-assisted filling, local squeeze, gate position; see porosity controls
Cold shut or flow line at a thin wallLeak along a line, often at a cornerWall section, fill time, die temperature at that corner
Machining breakthroughLeak appears only after the bore or face is cutMachining stock and bore depth on the drawing; CT sample after the cut
Insert or ejector pin interfaceLeak at a fixed point on the parting line or insert ringPin fit, insert preheat, seal land away from pins
Seal face distortion or fixture leakLeak moves between tests; passes on a second runSupport the wall, seal on a machined face, check the rig with a blank

If the leak is real and the cause is a pore path, the fix is either process or impregnation, not a higher test pressure. A casting that leaks 20 cc/min at 0.5 bar will not be saved by testing at 0.3 bar; it will just be shipped.

Fixtures cause more false rejects than castings

Seal on a machined face with a defined width, not on a cast skin. A cast surface has draft, parting-line mismatch and 0.3–1.0 mm of dimensional spread; an O-ring squeezed against it seals sometimes, which is the worst possible result for a 100% test.

Clamp force is the second trap. A 1.5 mm wall on a 200 mm housing deflects under the clamps, the seal face lifts on the far side, and the rig reports a leak the part does not have. Support the inside of the wall, or clamp on a boss designed for it. Keep chips and release agent off the seal; a chip under the O-ring reads exactly like a crack.

Then calibrate. A calibrated leak at the test pressure, run before the shift and recorded with the serial numbers, is the only thing that separates a real reject from a rig that has been drifting for a week. IATF auditors ask for that record, and so should you.

Aluminium die casting clamped in an air decay leak test fixture with a 0.6 bar gauge and leak tester display

What belongs on the drawing or the purchase order

Write the test as a specification, not as a sentence in an email.

Name the method and the standard behind it: bubble emission per ASTM E515, tracer gas per ISO 20485, or a plant method with the pressure and limit written out. Add the medium and its dew point for dry air, the pressure with a tolerance, the stabilise and measure times, the leak limit with its unit and the pressure it applies at, the surfaces that seal, and whether the test is 100% or sampled to an AQL.

Two more lines save arguments later: whether impregnation is allowed, and whether a failed part may be re-tested after a cure or must be scrapped. NADCA’s Product Specification Standards treat pressure tightness as a purchasable characteristic, which means the buyer has to state the level; the caster cannot guess it from “leak proof”.

Impregnation: a seal, not a repair of the wall

Vacuum impregnation fills connected porosity with a methacrylate or polyester resin and makes many leaking castings tight. It does not restore section, fatigue life or ductility, so it belongs on non-structural parts and on parts where the drawing allows it.

Mask threads, seal faces and any surface that is machined after impregnation; resin in a thread is a rejected part. Cure, then re-test at the same pressure and limit as the original test, not a lower one. For safety parts, structural nodes and anything welded after casting, the honest answer is usually no, and a process change is cheaper than a recall. The full decision path is in why die castings are impregnated.

One number puts it in perspective: at a 3% leak rate on a 5 cc/min limit, a 10,000-part month sends 300 parts to impregnation. If half of those come from one cavity or one gate, the die is the cheaper fix.

Sampling, retest and the reject rate

Safety and fluid-retention parts get 100% test. Brackets, covers and non-sealed housings can run on an AQL sample, but then the leak rate must be charted, not just passed or failed, or a slow drift stays invisible until a customer finds it.

Every retest gets a serial and a value. Two retests of the same part that pass after a fail are a signal about the fixture, not about the part, and they should be counted in the rejection and rework rate so the cost lands where it belongs.

FAQ

What pressure should an aluminum die casting be tested at?

0.3–1.0 bar of dry air for sealed housings, or 1.5× the maximum working pressure for a fluid channel. The number comes from the service condition and the fixture, not from a default.

Is air decay as reliable as helium testing?

For 1–10 cc/min on a production line, yes, if the temperature is stable and the rig is checked with a master leak. Helium goes three or four orders of magnitude tighter, at a cost and cycle time that only sealed or safety parts justify.

Can a leaking casting be repaired?

By impregnation, if the drawing allows it and the part is not structural or fatigue-critical. Welding a pore shut on a die casting usually creates a harder problem next to it.

Does passing a pressure test mean the part has no porosity?

No. It means no connected path reached the limit you set. Internal porosity still needs radiography or CT, with a level per zone, or it will show up after machining.